Propriedades de corrosão e caracterização química – metalográfica de próteses em aços inoxidáveis ISO 5832-9 e F138, removidas de pacientes
Loading...
Date
Authors
Journal Title
Journal ISSN
Volume Title
Publisher
Universidade Federal de Juiz de Fora (UFJF)
DOI
Abstract
This work has studied the chemical and metallographic composition (microstructure,
grain size, inclusion rate) of austenitic stainless steels which were developed to be applied as
biomaterials, and used in the production of orthopedical implants, removed from patients
which had been affected by inflammation; it has also been compared the sample surfaces, by
means of scanning electronic microscopy (SEM) after electrochemical attack. The results of
chemical analysis, performed by optical emission spectroscopy and Energy Dispersive
Spectroscopy (EDS) have shown that all samples are in agreement with the ASTM F138-92 e
ABNT NBR ISO 5832-9:2008 regulations, whereas the grain size has been determined by
optical microscopy and SEM. The surfaces of the samples were analyzed by SEM and EDS
techniques; samples were submitted to potentiodynamic cyclic polarization tests in 50 mV
potential after the passivation region in Ringer lactate and NaCl 0,9 mol.L-1 solutions at
36,5C; such SEM measurements were done to identify the type of corrosion over the
samples.
It has been concluded that all implants showed average grain sizes above the
recommended by the regulations; also the presence of delta ferrite in eight of the twelve
investigated implants has been seen, which according to the ASTM 138-92 regulation this
would not been possible even with a 100-fold increase at the optical microscope. It has also
been verified that in NaCl medium the ISO 5832-9 steel did not present any kind of localized
corrosion, instead of F 138 steel; in Ringer lactate solution, after 15 minutes attack at
1000mV/SCE, has been noted the presence of pits for ISO 5832-9 steel.
The cyclic polarization measurements have revealed that one of the investigated steels,
named ISO 5832-9, presented a very high resistance to localized corrosion when compared to
the F 138 samples, besides they did not release metallic ions to the electrolytic solutions. This
characteristic can be mainly attributed to the increasing of the passivation film stability, which
is also favored by the presence of nitrogen atoms in the solid solution composing the structure
of ISO 5832-9 steel. The pit corrosion tests have shown very useful to indicate the low
resistance to pit corrosion, present “in-vitro” in all the studied samples. The EDS mapping
analysis of F 138 samples, submitted to electrochemical attack in Ringer lactate medium, have
shown a loss of 63% of nickel and 26% of iron, when compared to the initial composition;
such metals were electrochemically solubilized to the Ringer lactate solution, where they can
probably precipitate from the solution, being a strong indication that the reactions taking place
in the patients have been motivated by these metal ions, which can be incorporated by the
human body.
The obtained results of this work are the basis of a tentative proposition to the
governmental organisms which are the responsible for the regulation of the technical
specifications for the prosthesis producers, requiring from them technical reports assuring the
quality for the implant pieces, i.e., for each manufacturing lot a description or a special
certificate containing the chemical composition and the metallographic characteristics
specified by the Brazilian laws.
Description
Keywords
Aços inoxidáveis , Implantes ortopédicos , Biomateriais , Corrosão , Curva de polarização , Microscopia eletrônica de varredura , Espectroscopia por dispersão de energia , Stainless steels , Orthopedical implants , Biomaterials , Corrosion , Polarization curve , Scanning electronic microscopy , Energy Dispersive Spectroscopy
Citation
Collections
Endorsement
Review
Supplemented By
Referenced By
Rights and licensing
Acesso Aberto