Abstract
Adhesive cementation of lithium disilicate veneers depends on two interfaces,
ceramic–cement and cement–enamel. Universal resin systems aim to simplify it by
incorporating silane into the adhesive and dispensing with phosphoric acid etching of
enamel, but it is unclear whether this simplification preserves bond strength and color
stability. This thesis evaluated the influence of enamel etching and silanization strategy
on these two outcomes in veneers cemented with a universal resin system. Two
randomized in vitro experiments were conducted with blinded outcome assessment. In
the mechanical experiment, 40 bovine enamel–lithium disilicate assemblies were
allocated to four groups (n = 10) in a 2 × 2 factorial design: non-etched enamel (E−) or
enamel etched with 37% phosphoric acid (E+), and ceramic treated only with the
silane-containing universal adhesive (SI; Scotchbond Universal Plus) or with prior
application of a separate ceramic primer (SS; RelyX Ceramic Primer). After
cementation with RelyX Universal and 10,000 thermal cycles, shear bond strength and
failure modes were evaluated. In the color experiment, 20 assemblies, all with etched
enamel, were allocated to SI or SS (n = 10) and stored in water for 90 days, and color
changes (ΔL*, Δa*, Δb*, ΔEab, and ΔE00) were calculated. Both enamel etching (p <
0.001; η²p = 0.841) and the separate primer (p < 0.001; η²p = 0.631) increased bond
strength, with no significant interaction between the factors (p = 0.162). Mean values
ranged from 5.95 ± 1.08 MPa (E−/SI) to 25.82 ± 4.58 MPa (E+/SS). Failure modes
differed among groups (p = 0.001): without etching, failures at the enamel–cement
interface predominated; with phosphoric acid, failures occurred mainly at the cement–
ceramic interface. In the color evaluation, nominal exploratory differences were
observed in ΔL* (p = 0.042) and Δa* (p = 0.008), with no difference in Δb*, ΔEab (p =
0.363), or ΔE00 (p = 0.277); an exploratory equivalence analysis (TOST) was
compatible with global equivalence between the strategies. In conclusion, for the
materials tested, the universal adhesive used alone did not reproduce the mechanical
performance of the separate ceramic primer, and omitting enamel etching markedly
reduced bond strength, whereas the global color change was similar between the
strategies. In the laboratory setting, maintaining phosphoric acid etching of enamel and
the separate ceramic primer maximizes bond strength.
Description