Influência de diferentes protocolos de polimento na rugosidade e adesão bacteriana em cerâmicas de dissilicato de lítio e silicato de lítio reforçadas com zircônia
Loading...
Date
Journal Title
Journal ISSN
Volume Title
Publisher
Universidade Federal de Juiz de Fora (UFJF)
DOI
Abstract
Ceramic restorations require adjustments before or after cementation. To restore
surface smoothness, reglazing or manual polishing is necessary; however, there is
controversy regarding the best method. Therefore, the aim of this study was to
compare surface roughness and bacterial adhesion on lithium disilicate and zirconiareinforced lithium silicate ceramics after different polishing protocols. Seventy-two
rectangular samples were fabricated for each ceramic group: Lithium disilicate (LD),
zirconia-reinforced lithium silicate - Vita Suprinity (VS), zirconia-reinforced lithium
silicate - Celtra Duo with firing (CD-AF), and zirconia-reinforced lithium silicate -
Celtra Duo without firing (CD). The samples were divided into six randomized groups
according to the protocol: Glaze (GL), Exacerapol (EX), Ceramisté (CR), Pk 5.1
Ceram (PK), Optragloss (OP), and Control (CO). Manual polishing protocols were
performed using abrasive rubber points with the same shape, in two- or three-step
processes, from different commercial brands. Roughness was assessed before and
after each protocol. Two representative samples from each group were evaluated
using scanning electron microscopy. Biofilm adhesion of Streptococcus mutans was
determined by colony-forming units per milliliter (CFU/ml). Statistical analysis was
performed using Jamovi software, employing two-way ANOVA followed by Bonferroni
post hoc test to identify significant differences between groups. A Pearson correlation
test was also conducted to evaluate the correlation between bacterial adhesion and
roughness in each ceramic group. The significance level was set at P = 0.05. A
significant interaction between ceramics and protocols was observed in terms of
roughness change (F(12,220) = 19.7, P < 0.006, η²partial = 0.517) and bacterial
adhesion (F(3,216) = 0.234, P < 0.872, η²partial = 0.003). The LD ceramic showed
the least roughness alteration, while CD had the highest. When evaluating only
protocols, there were significant differences between manual polishing protocols and
glaze. A large positive correlation was found between adhesion and roughness in all
groups: LD (r = 0.589, P < 0.001), VS (r = 0.6, P < 0.001), CD (r = 0.649, P < 0.001),
and CD-AF (r = 0.727, P < 0.001). For LD and VS, the most effective protocol was
OP, while for CD-AF and CD, it was PK. All ceramics showed less roughness
alteration with EX and CR protocols. For bacterial adhesion, significant differences
were only observed between ceramics under the GL protocol. Regarding roughness
alteration, all protocols except GL generated significant differences between
ceramics. The SEM analysis confirmed the roughness results. It was concluded that
all ceramics showed decreased roughness and bacterial adhesion after the different
polishing protocols but exhibited distinct behaviors when subjected to the same
polishing protocol.
Description
Keywords
Citation
Collections
Endorsement
Review
Supplemented By
Referenced By
Creative Commons license
Except where otherwise noted, this item's license is described as Acesso Aberto